Troubleshooting
Uneven wall thickness: five fixes, from free to expensive
Wall thickness problems are usually attacked with the most expensive tool first. Work through these five levels in order — most lines are fixed at level one or two, before anyone buys a controller.
Identify the pattern first
| Pattern | Where the material is | Usual cause |
|---|---|---|
| Eccentric | One side thick, the other thin at the same height | Parison off-center — die gap or mandrel |
| Top thin, base thick | Neck light, base heavy | Parison sagging — melt too hot or extrusion too slow |
| Top thick, base thin | Neck heavy, base light | Parison stretched — pre-blow too early |
| Local thin patch | One area white or bulged | Mold cooling uneven at that spot |
| Cyclic variation | Thick and thin alternate every few containers | Feed variation — regrind or screw slip |
Level 1: die gap (free)
Adjust the mandrel screws diagonally, a quarter turn at a time, and let three or four cycles run before measuring. This fixes eccentricity and nothing else. If the problem is top-to-base, the die gap is the wrong tool.
Level 2: process settings (free)
- Drop the melt temperature 3–5 °C to reduce sag.
- Move the pre-blow point later so the parison reaches the base before it is inflated.
- Raise blow pressure to push material into corners.
- Check cooling water temperature and flow — the mold is half of the wall thickness story.
Level 3: die head geometry (moderate)
Die land length, entry angle and flow path decide how evenly the melt reaches the gap. On multi-head machines, one head that runs thin points to a flow problem in that head rather than a machine setting. This is a change to the tooling, not to the recipe.
Level 4: parison wall thickness control (expensive)
A closed-loop controller moves the die gap during extrusion, so the parison can be thick at the base and thin at the shoulder. It is worth it when:
- Four cavities or more — cavity-to-cavity variation is otherwise uncontrollable.
- Containers over 5 L — the parison is long enough to sag measurably.
- Weight tolerance tighter than a few percent — the controller is also a material saver.
Level 5: container or mold redesign (most expensive)
Some shapes cannot be blown evenly: sharp shoulders, very long necks, deep handles. If levels 1–4 do not fix it, the geometry is the problem, and a small radius change often beats a machine change.
The cross-check that saves money
Before changing the machine, swap one variable:
- Run a known-good mold on the machine. If the wall is even, the problem is the mold.
- Run the problem mold on another machine. If the wall is even, the problem is the machine.
- Both uneven: process or material.
Two hours of swapping beats a month of guessing, and it tells you which quote to ask for.
Where to go next
- KSY105 and KSY120 drum machines — where wall thickness control earns its place
- Parison instability — the upstream cause of most wall problems
- Blow mold design — cooling layout and neck inserts
- Output calculation — why a heavier wall costs cycle time
Need a machine sized for your container?
Send the container size, weight, material and the output you need. We answer with a machine proposal and a capacity calculation, not a catalogue.