MATERIALS
UV and antistatic grades: when the additive changes the process
Additives are bought for what they do in service and then blamed for what they do in the extruder. UV stabilisers and antistats both change the way a bottle runs, and one of them changes it a lot.
UV stabilisers: small dose, small process effect
Three chemistries cover most outdoor work. UV absorbers, usually benzotriazoles or benzophenones, are dosed at 0.2–0.5% and do the job by absorbing the ultraviolet before it reaches the polymer. HALS at 0.1–0.5% work chemically instead, scavenging the radicals that light generates, and they hold color better. Carbon black at 1–2% is still the most effective protection for HDPE left in the sun, at the cost of a black bottle and extra heat build-up.
None of these normally moves melt viscosity much, which is why they are the easy additives. The complications are secondary. HALS is basic, so it can react with acidic pigment residues and shift the shade. UV absorbers can plate out on a hot die. Both are dosed low enough that a gravimetric feeder is the only way to hold them consistently.
Antistatic: the additive that rewrites the settings
Antistats work at the surface, not in the bulk. The molecule migrates out of the resin and attracts a thin film of atmospheric moisture, which lets charge drain away. Surface resistivity falls from around 10¹⁵ Ω to 10¹⁰–10¹² Ω, which is enough to stop dust attraction and static shocks.
The migration takes time: 24–72 hours after molding before the effect is fully there, so a bottle tested straight off the line will fail a surface resistivity check it would pass tomorrow.
- Glycerol monostearate is the common internal antistat at 0.1–0.3%. It is also a lubricant, so the screw slips, output drops 5–10% and weld lines weaken.
- Ethoxylated amines at 0.2–0.5% are more effective and more aggressive: they plate out on the die, smell faintly of amine and darken with heat.
- Conductive carbon black at 2–5% gives permanent, humidity-independent performance, and a black wall.
- Many antistats are not cleared for direct food contact, and migration limits apply even where they are.
What to watch on the machine
The first sign is a falling motor load and a shorter parison at the same screw speed. Resist the urge to raise melt temperature to bring output back, because heat increases migration and makes the plate-out worse. Raise screw speed instead, and accept a small output loss as the cost of the grade.
Printability is the second casualty. A lubricated surface holds ink badly, so check dyne level before printing and raise flame or corona treatment until it holds at 38 mN/m or above. Labels applied with adhesive fail at the edges first.
Store additive masterbatch sealed. Most carriers pick up moisture, and a wet batch gives silver streaks that look exactly like a dispersion fault.
Additive, effect, implication
Use the table to brief the machine operator, not just the buyer. Every one of these rows has a symptom someone will otherwise chase in the wrong place.
| Additive | Effect | Machine implication |
|---|---|---|
| HALS, 0.1–0.5% | Long-term light stability, low color | Possible die drool; check shade against standard |
| UV absorber, 0.2–0.5% | Blocks UV at the surface | Plate-out on a hot die; dose gravimetrically |
| Carbon black, 1–2% | Best outdoor protection | Higher melt temperature, longer cooling |
| GMS antistat, 0.1–0.3% | Surface conductivity after 24–72 h | 5–10% output loss, weaker weld lines |
| Ethoxylated amine, 0.2–0.5% | Strong, fast antistatic effect | Plate-out, amine odour, color drift |
| Conductive carbon black, 2–5% | Permanent conductivity | Harder melt, more torque, black wall only |
Where to go next
- Chemical containers — where antistatic performance is a handling requirement, not a nicety.
- Cosmetic bottles — color-critical work where a UV package must not shift the shade.
- Jerry can blow molding machine — outdoor containers that live or die on UV stability.
- Parison instability — what to check when output and parison length start moving.
- Blow molding materials — how additive grades sit inside the wider material choice.
Need a machine sized for your container?
Send the container size, weight, material and the output you need. We answer with a machine proposal and a capacity calculation, not a catalogue.