Troubleshooting
Parison instability: the seven settings that cause it
A parison that sags, necks down, surges or breaks is the most common complaint on an extrusion blow molding line, and almost always one of seven settings. Work through them in this order.
First, decide whether it is material or machine
| Symptom | Most likely cause | Check first |
|---|---|---|
| Parison gets thinner as it hangs | Melt too hot, or melt strength too low | Barrel and die temperatures |
| Thickness varies in a regular cycle | Screw slip, unstable feed, bridging in the hopper | Hopper, feed throat temperature |
| One side thick, one side thin | Die concentricity or off-center mandrel | Die gap, mandrel screws |
| Bubbles or black specks | Moisture, or material degrading in a hot spot | Drying, temperature profile |
| Parison breaks or surges | Too much regrind, or inconsistent regrind size | Regrind ratio and granulator screen |
The seven settings, in the order to adjust them
1. Temperature profile
The barrel should rise in steps to the die, and the die should be the hottest zone, not the coolest. If the parison sags, drop the die temperature about 5 °C and wait ten minutes before judging; if the surface is rough, raise it 5 °C. Change one zone at a time.
2. Screw speed and output
Faster screw speed adds shear heat, which raises melt temperature. Change screw speed and temperature together or not at all, otherwise you cannot tell which one fixed the problem.
3. Die gap and mandrel
Uneven gap gives an eccentric parison. Adjust the mandrel screws diagonally, a quarter turn at a time, and let three or four cycles run before measuring again.
4. Wall thickness programme
If the machine has parison control, check that the profile matches the container. A profile set for another container will look like instability.
5. Material and regrind
Regrind above about 30% starts to show as feed variation. Keep granulator screen size consistent; mixed fine and coarse regrind feeds unevenly.
6. Feed section
Bridging in the hopper and a hot feed throat are the two hidden causes. Check the hopper dryer and the cooling water on the feed throat.
7. Pre-blow
Pre-blow pressure that fluctuates makes the parison move before the mold closes. Check the regulator and the valve response, not the parison.
A five-minute check sheet
- Barrel and die temperatures against the recipe
- Screw current steady, not hunting
- Die gap even on both sides
- Mandrel screws tight
- Hopper free-flowing, resin dry
- Regrind ratio within the recipe
- Pre-blow regulator steady
- Parison control profile matches the container
Where to go next
- Uneven wall thickness — the next symptom to chase once the parison is stable
- Maintenance schedule — most instability starts with a maintenance item
- Scrap recycling — regrind ratio and consistency
- KSY machine range — screw and die head sizes for your container
Need a machine sized for your container?
Send the container size, weight, material and the output you need. We answer with a machine proposal and a capacity calculation, not a catalogue.