Process
Start-up and shutdown: a procedure that protects the screw
Most screw damage happens in the ten minutes around a stop, not during production. A fixed soak time and a written stop routine cost far less than one barrel repair.
Soak time is not optional
When the heater bands reach set point the barrel is hot on the outside and still cold in the flights. The screw, the non-return valve and the die head all need time to catch up.
- Small machine: 20–30 minutes at temperature before the screw turns.
- Large machine or a long barrel: 45–60 minutes.
- Probe the barrel with a contact thermometer rather than trusting the controller display. A 10 °C gap means keep waiting.
- Turn the screw by hand, or inch it at 5 rpm, before it runs under load.
Never start cold
Starting a cold screw is how you shear a screw tip, strip a drive key or load a thrust bearing. The plastic in the flights is solid; the torque has to go somewhere, and it goes into the weakest part of the drive train.
Interlocks help, but the useful rule is simpler: barrel at temperature, soaked, and the screw turning freely in inch mode before the heat is switched to run.
Then purge. Three to five shots of production material, until the parison is clean and the surface is uniform. Use a purging compound only if the last material in the barrel was heat-sensitive.
Stops are not all the same
- Under 30 minutes: hold temperatures, keep the barrel full, turn the screw for ten seconds every ten minutes.
- Weekend: purge, leave the barrel full of production material, hold set points. If the shop is cold, expect the die head to lag on restart.
- Long stop: purge with compound, empty the barrel, then switch off. Never leave a heat-sensitive material sitting at temperature.
- In every case: never leave the screw stalled against cold plastic under full torque.
Start-up and shutdown, step by step
| Step | Start-up | Shutdown |
|---|---|---|
| Heaters | On at full power, watch every zone rise together | Off only after the barrel is purged and empty |
| Soak | 30–60 min at set point, probe the barrel | Not applicable |
| Screw | Turn by hand, then inch at 5 rpm | Run out the last shot, leave the screw forward |
| Purge | Three to five shots until the parison is clean | Purge with compound, then empty the barrel |
| Mold water | On 15 minutes before the first shot | Off once the mold is below 40 °C |
| Air | Drain the filter, check pressure at the blow pin | Drain the receiver, close the supply valve |
| Die head | Check the first parison for cold slugs | Leave the die gap open |
| Record | Log zone temperatures and first-off weight | Log the reason for the stop |
What the log is for
Write down zone temperatures, the soak start time, the first-off weight and the reason for the stop. Three months of that record shows a heater band drifting long before it fails, and it turns an argument about a bad batch into a five-minute check.
A start-up that takes forty minutes longer than it should is usually a soak that was never timed, or a die head that was never checked for a cold slug.
Where to go next
- Maintenance schedule — the weekly checks that keep a start-up uneventful.
- Service and support — what to do when a barrel or screw is already scored.
- Machine range — barrel size and heating zones differ, and so does the soak time.
- Scrap recycling — where purge lumps and start-up scrap should end up.
Need a machine sized for your container?
Send the container size, weight, material and the output you need. We answer with a machine proposal and a capacity calculation, not a catalogue.