Materials
PETG thick-wall bottles: why the base is the hard part
A PETG bottle with a heavy base looks like a simple shape and is one of the harder things to run consistently. The problem is not the wall — it is getting a thick base to cool without crystallising, sinking or cracking.
What is different about PETG
- It is amorphous. PETG does not crystallise like PP or HDPE, which is why it stays clear — and why it stays soft for a long time after the mold opens.
- It is hygroscopic. The resin absorbs moisture and must be dried before extrusion, or the wall shows bubbles and streaks.
- It has a narrow processing window. Too cold and the parison is dull with unmelt; too hot and it droops and sticks to the die.
- It scratches. Automatic de-flashing and rough take-out leave marks that are visible through the wall.
Why the base is the problem
A thick base holds heat. The wall may be cool enough to eject while the base is still soft, so the base sinks on the conveyor or deforms under its own weight in the case. Push the cooling to fix that and the base surface takes on a crystalline haze or internal voids.
| Symptom | Usual cause |
|---|---|
| Base sinks after ejection | Base still hot when the mold opens; cooling time set by the wall, not the base |
| White haze in the base | Over-cooling or excessive blow pressure on the base insert |
| Bubbles or streaks | Resin not dried, or moisture picked up in the hopper |
| Cracks at the base corner | Sharp internal radius plus residual stress |
| Visible sink mark on the base | Base insert too hot, or insufficient packing time |
What the machine has to do
- Dedicated screw and die head for PETG. A general-purpose HDPE screw shears PETG too hard.
- Independent base cooling. The base insert needs its own circuit, colder than the body, with enough flow to pull heat out of the thick section.
- Slow, controlled blow. PETG needs a gentler inflation than HDPE to avoid marking the base.
- Longer cycle. Accept it. A thick-base PETG bottle runs at a fraction of the rate of the same volume in HDPE, and quoting otherwise is how projects fail.
Mold details that decide the result
| Detail | Recommendation |
|---|---|
| Base insert material | Beryllium copper for heat transfer, polished to a mirror finish |
| Base corner radius | Generous, not sharp — sharp corners concentrate stress and crack |
| Base cooling | Separate circuit, baffled close to the base cavity |
| Body cooling | Separate from the base, so the two can be set independently |
| Neck insert | Beryllium copper, independent circuit; the neck sets the seal |
| Surface finish | Polished in the draw direction; any cross-polish shows through the wall |
Setting the line
- Dry the resin to the supplier’s figure, and keep the hopper dryer running.
- Bring the barrel up to temperature and let it soak; PETG needs longer to stabilise than HDPE.
- Set the cycle from the base, not the wall: run until the base is dimensionally stable on ejection, then check the wall.
- Adjust parison thickness so the base gets the material it needs without over-packing the body.
- Check the base on a cut section, not by eye — sink and internal voids are invisible from outside.
Where to go next
- KSY45-J1.8L PETG machine — dedicated screw and die head for clear bottles
- Cosmetic bottles — what the personal care market asks of the wall
- Bottle molds with neck inserts — beryllium copper inserts and cooling layout
- HDPE or PP — whether PETG is really the material you need
Need a machine sized for your container?