Process
Parison programming: how a wall thickness profile is built
A parison programme is only as good as the profile behind it. Here is what the controller actually moves, how many points you need, and how to read the result on a cut section instead of guessing.
What the programme actually moves
The controller does one thing: it moves the die gap while the parison leaves the head. A section of the bottle that needs less material gets a narrower gap; a neck shoulder, a handle root or a base corner gets a wider one. Points, ramps and offsets are bookkeeping around that single movement.
On a continuous extruder the programme runs on a timer tied to the extrusion cycle. On an accumulator machine it runs on ram position, which repeats better because it does not care how fast the ram travelled.
- You are programming flow, not wall. The wall is what the flow becomes after swell, stretch and blow.
- The gap that counts is at the die lip. A 2 mm gap on hot HDPE can deliver more than 2 mm of wall once swell is included.
- Confirm which end of the parison point 0 refers to before you change a number. Controllers differ, and one reversed profile costs a shift.
Ten to twenty points is the useful range
Fewer than ten points and the interpolation becomes visible: the wall steps between measuring positions, and you cannot fix one thin band without moving a broad area. More than twenty and you are usually fitting the controller to measurement noise.
- Wall measurement repeats to about ±0.1 mm. A change that moves less than 5% of the wall is below the noise.
- Put points where the geometry changes: neck shoulder, start of the label panel, handle root, base radius.
- Leave the straight body on two or three points. It does not need more.
Build the profile in this order:
- Run flat at 100% and keep the bottle.
- Cut it on the center line and measure at eight heights.
- Mark the two thinnest bands and the two thickest.
- Move only the points at the thin bands, in 5% steps.
- Re-run three bottles, measure again, and stop when the spread is inside ±10%.
Reading a cut section
A single wall reading tells you almost nothing. Cut the bottle and look at four things:
- Whether the thinnest point sits where the programme says it should.
- Whether the thin band runs right round the circumference or only on one side.
- Whether the pinch-off weld is intact and the base corner is filled.
- Whether the front and back walls agree with each other.
If the band follows the points, it is a profile problem. If the same clock position is thin on every bottle, it is a die or heat problem: mandrel off center, a cold spot on the head, a dead heater band. If the whole parison drifts over twenty minutes, look at temperature and material before you touch the programme.
Profile problems and die problems
The two look similar on a bad bottle and need opposite fixes. The table separates them.
| Symptom | Likely cause | Correction |
|---|---|---|
| Thin band at one height, all round | Point set too low | Raise it 5% and re-check the two neighbours |
| Thin on one side only | Mandrel off center or a cold spot on the head | Check concentricity and heater bands first |
| Thick shoulder, thin body | Too many points stacked at the top | Spread the upper points over a longer stroke |
| Visible step between two heights | Gap in the point interval | Add one point and blend the ramp |
| Base corner not filled | Profile too lean at the base, or low blow pressure | Add 5–8% at the base point, then check pressure |
| Weak weld at pinch-off | Gap too wide at the base | Close the last points; do not raise pressure to hide it |
Where to go next
- Wall thickness control — the measurement side of the same job, including where to cut and how often to check.
- Parison instability — for when the profile is right but the parison will not hold its shape.
- Blow mold tooling — die and mandrel work, if concentricity turns out to be the real problem.
- HDPE bottle machines — how the extrusion and clamping side is laid out on the machine itself.
Need a machine sized for your container?
Send the container size, weight, material and the output you need. We answer with a machine proposal and a capacity calculation, not a catalogue.