Extrusion blow molding machines, molds and line equipment for 5 ml bottles to 25 L jerry cans

KESYER KSY blow molding machinery

Process

How much blow pressure is enough

Pressure is the easiest variable to change and the easiest to overdo. Here is what the air actually does, where the useful range sits by container size, and how to tell too little from too much.

What the air actually does

Blow pressure has three jobs: expand the parison against the mold wall, press the plastic into the fine detail of the neck and base, and hold the wall against cooled steel long enough to set the shape. It does not thin a heavy wall in any useful way, and it does not compensate for a cold mold.

The gauge is not the parison. Every metre of hose, every filter and every quick coupling costs pressure. A 0.7 MPa reading at the regulator can be 0.45 MPa at the blow pin when the bore is small and the valve is slow. Measure at the pin, not at the panel.

Pre-blow and final blow are different tools

  • Pre-blow at 0.2–0.4 MPa inflates the parison into a rough preform and stops it collapsing on the way into the mold. It also stretches the material while it is still hot, which is where an even base comes from.
  • Final blow at 0.4–0.8 MPa does the detail: thread, handle, base radius, lettering.
  • Pre-blow timing matters more than pre-blow pressure. A pre-blow that starts 20 ms late makes a different bottle.
  • On thick-wall work a long, soft pre-blow beats a hard final blow.

Typical final blow pressure by container

The numbers below are shop ranges for HDPE and PP, not machine limits. They move with mold temperature, parison temperature and the bore of the blow pin.

Container Typical wall Final blow
Cosmetic bottle, 50–200 ml 0.5–0.8 mm 0.6–0.8 MPa
Detergent or shampoo, 500 ml–1 l 0.8–1.2 mm 0.5–0.7 MPa
Jerry can, 5–10 l 1.5–2.5 mm 0.4–0.6 MPa
Drum, 20–30 l 3–5 mm 0.3–0.5 MPa
Wide-mouth food jar 1.0–1.5 mm 0.5–0.7 MPa
Thick-wall PETG bottle 2–4 mm 0.5–0.7 MPa

Why more pressure is not better

  • Stress: every extra 0.1 MPa packs more material into the pinch-off and leaves a whitened weld that fails in a drop test.
  • Marks: over-pressure prints the vent tracks and every polished defect into the surface.
  • Flash: past a point the clamp cannot hold the extra force and flash appears at the parting line. The usual reaction is to raise pressure again to fill a corner, which adds more flash.
  • Air and time: more pressure means more air to vent before the mold opens, and venting is dead time in every cycle.

There is also a floor. Below roughly 0.25 MPa the parison may not reach the far corners of a wide part at all, and the surface stays dull wherever the plastic never touched steel.

How to tell you have too little

  • Base radius rounded instead of crisp.
  • Thread not fully formed on one side of the neck.
  • Dull patches where the plastic never touched the steel.
  • Handle web not welded through.

Raise in 0.05 MPa steps, stop when the detail appears, then take one step back. If the detail still will not come at 0.8 MPa, the problem is air flow rather than pressure: check the valve, the bore and the exhaust port.

Where to go next

  • Flash and neck faults — where over-pressure usually shows up first, and what else causes the same look.
  • Blow molds — venting and pinch-off design, the other half of a clean parting line.
  • Jerry can machines — larger parts where volume flow matters more than gauge pressure.
  • Leak testing — how to test the result instead of judging it by eye.

Need a machine sized for your container?

Send the container size, weight, material and the output you need. We answer with a machine proposal and a capacity calculation, not a catalogue.

Send your container