MATERIALS
Drying resin: which materials need it and what happens if you skip it
HDPE does not need drying and PETG does. Confusing the two is the quickest way to a wall full of bubbles, and the bubbles usually appear after the mold has been blamed.
Hygroscopic or not
The split is simple and it is not about how the pellet looks. Polyolefins — HDPE, LDPE and PP — do not absorb water into the polymer. Any moisture sits on the surface, and on washed flake that can still be 0.1–0.3%, enough to matter. A vented barrel or an hour at 80 °C removes it.
Engineering and clear resins are different. PETG, PET, PA6, PA66, PC, EVOH and TPU bind water inside the pellet, and only dry air pulls it back out. PVC sits in between: surface moisture only, and it must not be dried hot enough to degrade.
A working rule: if the resin is clear or engineering, dry it; if it is a polyolefin, dry only the flake that came off a wash line.
What moisture does inside the wall
Water that enters the extruder as bound moisture turns to steam as the resin melts. PETG also hydrolyses, so the chain length drops at the same time as the bubbles form, and the bottle goes brittle before it goes visibly wrong.
The volume argument is worth doing once. A 0.1% moisture level in a 50 g shot is 50 mg of water, which becomes roughly 100 ml of steam at melt temperature — about the volume of the parison itself. It has nowhere to go except into the wall.
- Bubbles and voids, often only visible on the inside surface.
- Silver streaks on the outside, which look like a screw problem.
- Weak weld at the pinch, and drop test failures that come and go with the weather.
- For EVOH, a barrier layer that no longer meets its oxygen target.
Hopper dryer or dehumidifying dryer
A hopper dryer blows hot air through the resin. Its dew point follows the room, usually around 10–15 °C, so it can lift surface moisture but it cannot dry PETG. It is cheap, simple and perfectly adequate for washed HDPE flake.
A dehumidifying dryer passes air over a desiccant bed and delivers it at −20 to −40 °C dew point. That is what PETG, PA, PC and EVOH need, because a dry atmosphere is the only thing that pulls bound water out of the pellet.
Sizing matters as much as temperature. A dryer that is too small for the throughput never reaches the target moisture, even with the controller set correctly, because the airflow per kilogram of resin is too low.
- PETG softens and sticks together above about 75 °C. Do not borrow a PA drying recipe for it.
- Insulate the hopper and keep the lid closed; resin left open overnight reabsorbs what you just removed.
- Log dew point weekly and replace desiccant on condition, not once a year.
Dry to a number, not a timer
Drying schedules are starting points. The only proof is a moisture reading from the pellet, taken with an analyser just before the hopper. Dry only what the shift will run, and do not cycle resin wet and dry repeatedly.
| Material | Hygroscopic | Drying temperature | Time | Target moisture |
|---|---|---|---|---|
| HDPE | No, surface only | 80 °C, flake only | 1–2 h | Surface dry |
| PP | No, surface only | 80 °C, flake only | 1–2 h | Surface dry |
| PVC | Surface only | 60–70 °C | 1–2 h | Not critical |
| PETG | Yes | 65–70 °C | 4–6 h | 0.04% or less |
| PET | Yes | 160–170 °C | 4–6 h | 0.005% or less |
| PA6 | Yes | 80–100 °C | 4–6 h | 0.10% or less |
| PC | Yes | 120 °C | 3–4 h | 0.02% or less |
| EVOH | Yes | 60–65 °C | 2–4 h | 0.30% or less |
Where to go next
- PETG blow molding machine — the machine side of a resin that will not run without a dryer.
- PETG thick-wall bottles — why thick walls make moisture faults more visible, not less.
- Parison instability — separating a moisture fault from a screw or temperature fault.
- Food and milk bottles — the containers where a bubble in the wall is a shelf-life problem.
- Auxiliary equipment — dryers, chillers and the rest of what sits around the machine.
Need a machine sized for your container?