Most color faults are not pigment faults. They are dosing position, mixing and a dead spot in the die head, and the fix is usually mechanical rather than chemical.
Let-down ratio and where you dose it
Blow molding normally runs at 1.5–3% let-down. Pale tints sit at the low end, whites and saturated darks at the top. A masterbatch carries 20–50% pigment in a carrier resin, and the carrier should match the base resin: a PE carrier in HDPE, not a universal carrier that happens to disperse everything.
Gravimetric dosing holds about ±0.5%. Volumetric dosing drifts by roughly ±5% as the regrind ratio and bulk density change, which is enough to see between the first and last hour of a shift.
- Dose at the feed throat with the virgin pellets, never into the metering zone where there is no length left to mix.
- Match pellet size to the resin. Fines and dust in the masterbatch streak before the pigment does.
- Keep the let-down steady when the regrind ratio changes, or the color will drift with it.
Why streaks happen
Streaks are unmixed material, and there are only a few places it can hide.
- Dispersion. Pigment agglomerates above 20–30 µm read as specks. A cold screw, short residence time and low back pressure all leave them intact.
- The screw. No mixing section, or one worn past its clearance. A slotted flight or Maddock-style mixer fixes it and raises melt temperature by a few degrees, which you then have to cool elsewhere.
- Dead spots in the die. A scratch, a step at a joint, a thermocouple pocket. Material hangs there, degrades and releases in a slug, which is the comet tail you see running down one side of the bottle.
- Moisture. Wet masterbatch gives silver streaks, not color streaks, and it is easy to misdiagnose.
- Over-lubricated masterbatch. It plates out on the die, dulls the surface and slowly closes the flow area.
Color change: the sequence and the real time
A color change is a purge job, not a switch. Run natural resin until the parison is clean, run a purging compound, then strip and clean the die head if you are going from dark to light. Only then introduce the new color, run 10–20 shots to stabilise, and check the first bottles under D65 light rather than factory lighting.
On a two-cavity machine at a 12-second cycle, light to light takes 15–25 minutes and 2–5 kg of material. Dark to light with the die open takes 40–70 minutes and 8–15 kg. Those numbers barely move with a better masterbatch; they move when you schedule light to dark across the shift instead of fighting the sequence.
Keep a log of color, purge time and shots to stable. After three changes the log tells you your own real number, which is more useful than any supplier claim.
Defect to cause
Start with the physical evidence on the bottle before changing the formulation. Nine times in ten the defect points at one location.
| Defect | Likely cause | First check |
|---|---|---|
| Longitudinal streaks | Poor dispersion or a cold screw | Melt temperature, mixing section |
| Swirls and marbling | Dosing position or segregation | Feeder, pellet size match |
| Dark specks in one line | Dead spot in the die head | Strip and inspect the flow channel |
| Color strength drift | Volumetric dosing | Weigh masterbatch over 100 shots |
| Band at the weld line | Carrier does not match the base resin | Check carrier against resin type |
| Dull surface, plate-out | Over-lubricated masterbatch | Reduce let-down, check the formulation |
Where to go next
- Detergent and shampoo bottles — the color-critical work where a streak means a rejected bottle.
- HDPE bottle blow molding machine — screw and head options that decide how well color mixes.
- Daily chemical bottle molds — where a polished flow path removes a whole class of color faults.
- Blow molding line configuration — how dosing and feeding fit into the line around the machine.
- Blow molding materials — the material context for masterbatch and carrier choice.