Extrusion blow molding machines, molds and line equipment for 5 ml bottles to 25 L jerry cans

KESYER KSY blow molding machinery

Applications

Blow molding machines for detergent and shampoo bottles

HDPE and PP bottles for shampoo, shower gel, laundry detergent, dish soap, bleach and toilet cleaner, from 300 ml to 5 L.

HDPE detergent bottles

Containers

Household chemical bottles

Detergent bottles are large-volume products with handles, angled necks and strong colors. They need stable wall thickness and leak-free necks.

  • Shampoo and shower gel bottles
  • Laundry detergent bottles with handles
  • Dish soap and bleach bottles
  • Toilet cleaner bottles with angled necks

Engineering

What makes a detergent bottle hard

A detergent or shampoo bottle is the container a customer squeezes, so it is judged by the hand rather than by a caliper. It has to spring back after being squeezed flat, hold its shape on a shelf with a label wrapped around it, and survive a case drop without splitting along the seam. Three requirements, and they are mostly in conflict.

Spring-back is a wall thickness and wall distribution question. A bottle that is too stiff will not dispense; one that is too soft dents in the crate and looks damaged before it is opened. In practice a 1 L shampoo bottle lands at 0.7 – 1.0 mm on the body with a slightly thicker shoulder, and the panel design does the rest: a waist or a pair of ribs gives the squeeze without adding material.

The handle is the second problem. Above 2 L most detergent bottles are handled, and the handle is formed by the mould pinching the parison rather than by a separate part. Where the pinch happens the wall is stretched, so the handle root is the thinnest section of the container and the first place a drop test finds a crack. Moving the handle to the parting line, and feeding the root from a thicker part of the parison, is what fixes it.

The third is the view strip. A transparent window on an opaque bottle is a mould insert with a polished face, and the resin flowing across it has to stay clear: any weld line or trapped air shows as haze. It is a mould and die-head temperature job more than a machine job, which is why the same machine can make good bottles on one mould and hazy ones on another.

Range

Container range and what it demands

Weights below are typical for HDPE at the wall the application needs; PP runs slightly lighter for the same stiffness.

ContainerTypical weightNeckWallWhat decides the design
300 – 500 ml shampoo bottle22 – 35 g28 mm0.6 – 0.9 mmSqueeze recovery; flat label panel
750 ml – 1 L shampoo or lotion40 – 60 g28 – 33 mm0.7 – 1.0 mmPanel stiffness; neck squareness for the cap
1 – 2 L handled detergent70 – 110 g33 – 38 mm0.8 – 1.2 mmHandle root; base for stacking in a crate
2 – 3 L handled detergent100 – 150 g38 – 43 mm1.0 – 1.4 mmHandle strength; top load in a two-high stack
3 – 5 L fabric softener or bleach140 – 210 g38 – 45 mm1.1 – 1.5 mmBase corner; chemical resistance of the resin
View-strip bottle, any size+5 – 8%as aboveas aboveInsert polishing; flow across the window

Typical values for single-layer HDPE. Clarified PP gives a translucent bottle at a lower weight but with a narrower processing window.

Selection

Choosing the machine by container size

The table uses our current model range and production cycles for HDPE — extrusion, blow and cooling, not the dry cycle. Shot weight is the mass of one complete cycle and is what the screw has to deliver.

ContainerModelDie heads × stationsShot weightCycleOutput per hour
300 – 500 ml shampooKSY55-J2.5L3 × 2 = 60.13 – 0.21 kg20 – 26 s830 – 1,080
750 ml – 1 L shampooKSY65-J3L2 × 2 = 40.16 – 0.24 kg26 – 32 s450 – 550
1 – 2 L handled detergentKSY85-J10L1 × 2 = 20.14 – 0.22 kg28 – 36 s200 – 255
2 – 3 L handled detergentKSY85-J10L1 × 2 = 20.20 – 0.30 kg32 – 40 s180 – 225
3 – 5 L softener or bleachKSY95-J12L1 × 2 = 20.28 – 0.42 kg36 – 46 s155 – 200

Output = 3,600 ÷ cycle × containers per cycle, calculated. A handled container is heavier than a round bottle of the same volume, so it runs on a heavier platform and a longer cycle.

The row people question most is the 1 – 2 L one: a 2 L bottle on a 10 L platform looks oversized. It is not. The handle and the wide shoulder need a parison large enough to fill both, and the platens have to open far enough for the handle to clear the mould. A smaller platform can close the mould but cannot give the handle its wall.

Process

The process window

ParameterTypical settingWhat goes wrong outside it
Melt temperature, HDPE175 – 195 °CAbove: sag and a thin shoulder. Below: unmelted particles and a rough panel
Melt temperature, clarified PP190 – 210 °CAbove: the clarifying agent loses effect and the bottle hazes
Mould temperature10 – 16 °CWarm: longer cycle and a glossy surface that shows every mark
Blow pressure0.4 – 0.7 MPaLow: soft corners and a view strip with trapped air
View-strip insert temperature2 – 4 °C below the bodyEqual: haze at the window edges and a visible weld line
Handle pinch landSharp, 0.2 – 0.3 mm clearanceWorn: a web across the handle that has to be cut by hand

The view strip is the setting that gets blamed for a mould problem. The window is formed where the parison is pressed against a polished insert, so the resin there must be at a temperature that still flows: 5 °C colder and the weld line becomes visible as a white line across the window. If a mould hazes in one cavity only, the answer is the insert, not the machine.

Quality

Tests that decide acceptance

TestWhat it provesWhere it typically fails
Squeeze and recoveryThe bottle dispenses and returns to shapePanel too thick, or the waist in the wrong place
Drop, filled, on a cornerThe seam and the handle survive handlingHandle root and base corner
Top load, stacked two or three highThe crate stack does not deform the bottleShoulder ring and the cap seat
Label adhesion and panel flatnessThe wrap label sits without bubblesPanel curvature; mould temperature too high
View-strip clarityThe product is visible through the windowWeld line, trapped air, insert polish
Cap torque and sealThe closure holds in transitNeck ovality after blowing

Troubleshooting

Defects and where they come from

What you seeUsual causeWhat to change first
Bottle dents when squeezedPanel unsupported, wall under 0.6 mmAdd a rib, or thicken the panel to 0.7 mm
Does not spring backWall too thick at the waist, or the resin too stiffThin the waist by 0.1 mm, check the melt index
Handle root cracks on dropHandle pinched from a thin part of the parisonMove the handle to the parting line, thicken the root
Hazy view stripInsert too cold or not polishedWarm the insert 3 – 5 °C, repolish
White line across the windowWeld line formed at the insert edgeMove the gate position, adjust the parison profile
Label bubbles after a weekBottle still relaxing; mould too warmDrop mould temperature 3 °C, extend cooling

Line

Line configuration and a worked example

ItemSpecification for a 1 L shampoo line
Blow molding machineKSY65-J3L, Ø60 / Ø65 mm screw, two die heads, double station
MouldTwo cavities, chrome-plated cavity, polished view-strip insert, hardened pinch land
De-flashingOne unit per station, cutting against the mould
ConveyorAccumulation before the labeler so a stoppage does not stop the machine
Chiller and granulatorAir-cooled chiller; granulator returning flash to the hopper at a fixed ratio

Worked example: a 1 L shampoo bottle at 55 g, four cavities, 30 s cycle. Shot weight is 4 × 0.055 = 0.22 kg, so the plasticising demand is 0.22 ÷ 30 s = 26 kg/h — well inside the 50 – 60 kg/h of the KSY65-J3L. Output is 3,600 ÷ 30 × 4 = 480 bottles an hour, or 26 kg of HDPE.

Push the same mould to 20 s and the arithmetic says 720 an hour, but the screw is now asked for 40 kg/h and cooling has not been given enough time: the bottles come out warm, the panels bow as they cool, and the label line rejects them a day later. The cycle that matters is the one measured on the conveyor, not the one on the machine's display.

Evidence

From projects we have built

A view-strip bottle line in Indonesia runs two die heads on a double station, with the transparent window formed by a polished insert in each cavity. The project notes cover what the window does to the cycle and why one cavity hazed while the other did not. View-strip bottles on a two-head line.

For the container families behind these numbers see the case studies index, and for the arithmetic how to calculate blow molding output.

KSY65-J3L in a bottle production workshop.

See it running

KSY65-J3L in a customer workshop

A KSY65-J3L producing household bottles with take-out and conveyor.

FAQ

Questions

HDPE or PP for a detergent bottle?

HDPE for most household detergents: it is tougher in the drop test and cheaper. PP where the product is warm or the bottle needs a stiffer, glossier surface. Clarified PP gives a translucent look at a slightly higher cost.

Can you blow a bottle with a transparent view strip?

Yes. The window is a polished insert in each cavity, and the resin flowing across it has to stay clear. It is a mould and die-head temperature job, which is why the same machine can make clear windows on one mould and hazy ones on another.

How thick should a 1 L shampoo bottle be?

Typically 0.7 – 1.0 mm on the body, slightly thicker at the shoulder, at a weight of 40 – 60 g. Below about 0.6 mm the bottle dents in the crate; above 1.1 mm it stops springing back when squeezed.

Why does my bottle dent after a week in the warehouse?

The crate stack is carrying the load through a panel that was designed for squeezing, not for stacking. The fix is usually a rib or a thicker shoulder, not a thicker body.

Which machine for 2 L and 3 L handled detergent bottles?

KSY85-J10L for 1 – 3 L handled containers, KSY95-J12L above 3 L. The handle sets the platform more than the volume does, because the parison has to fill the handle and the body at the same time.

Can the same machine run shampoo bottles and 5 L softener?

Mechanically yes, economically rarely. A machine sized for 5 L runs small bottles slowly, and the mould change between them costs more than the machine saves.

How much regrind can go back in?

20 – 30% on hidden parts of a single-layer bottle. Keep it lower on a view-strip bottle, because regrind shows in the window as a colour shift.

Do you supply the mould with the machine?

Yes, quoted together. The neck insert and the pinch land are specified separately, because those two decide whether the cap seals and whether the handle has to be trimmed by hand.

Get a quote

Send us your container

Send the drawing or a photo with volume, weight and material, and the output you need. We recommend the machine and mold.

We reply within one working day. Your details are only used to answer this inquiry.