Materials guide
Extrusion blow molding materials: properties, processing and how to choose
Which plastics can be extrusion blow molded, how each one behaves in the machine, and which material and layer structure suits your product. Our machines process HDPE, LDPE, PP, PVC and PETG, EVOH and PA barrier layers, and on custom machines ABS, TPE, TPU, EVA, PS and K-resin.
Overview
Blow molding materials compared
The material decides the screw, the die head, the temperatures, the cooling time and therefore the output. These are the materials used most in extrusion blow molding.
| Material | Density, g/cm³ | Barrel temperature | Mold shrinkage | Drying | Appearance | Typical containers | KSY machine |
|---|---|---|---|---|---|---|---|
| HDPE | 0.94 – 0.965 | 170 – 210 °C | 1.5 – 3.0 % | Not needed | Opaque to translucent | Milk, detergent, chemical, oil and pesticide bottles, jerry cans, drums | All standard models |
| LDPE | 0.91 – 0.93 | 150 – 190 °C | 1.5 – 3.0 % | Not needed | Translucent, soft | Squeeze bottles, eye-drop and dropper bottles | KSY50-J2L |
| PP | 0.90 – 0.91 | 190 – 230 °C | 1.0 – 2.5 % | Not needed | Translucent, glossy | Hot-fill food, pharmaceutical and cosmetic bottles, wide-mouth jars | PP machines |
| PVC (rigid) | 1.30 – 1.40 | 160 – 190 °C | 0.2 – 0.6 % | Usually not needed | Clear, stiff | Clear household, glue and cosmetic bottles | Standard models with PVC screw and die |
| PETG | about 1.27 | 210 – 250 °C | 0.2 – 0.5 % | Required, about 65 °C for 4 – 6 h | Glass-like clarity | Clear cosmetic and personal care bottles, handled clear bottles | KSY45-J1.8L |
| EVOH (barrier layer) | 1.12 – 1.20 | 200 – 230 °C | — | Required | Thin inner layer | Oxygen barrier for food, sauces, pharmaceuticals | Multilayer machines |
| PA (barrier layer) | about 1.13 | 230 – 260 °C | — | Required | Thin inner layer | Solvent barrier for agrochemicals and chemicals | Multilayer machines |
Typical values for extrusion blow molding grades. Always follow the data sheet of your resin supplier; barrel temperatures are set lower at the feed zone and higher towards the die head.
HDPE
HDPE: the standard material for bottles and cans
High-density polyethylene is used for most extrusion blow molded containers. It has high melt strength, so the parison hangs without sagging, and it is forgiving to process.
Properties
- Stiff and tough, good drop impact resistance
- Resistant to most acids, alkalis, detergents and oils
- Good moisture barrier, poor oxygen barrier
- Natural color is milky translucent; easy to color
Typical containers
- Milk jugs and juice bottles
- Shampoo, detergent and bleach bottles
- Engine oil and lubricant bottles
- Pesticide bottles, 5 – 25 L jerry cans and drums
Processing notes
- Runs on the standard HDPE screw of every KSY model
- Parison sag shows when the melt is too hot or the parison very long; lower the temperature or use parison control
- Shrinks 1.5 – 3 % after molding; the mold is cut oversize to give the right volume
- Cooling time sets the cycle; mold water at 10 – 15 °C with a chiller shortens it
Common problems
- Uneven wall: center the die and check heater bands
- Warped bottles: longer cooling or colder mold water
- Stress cracking with some detergents: choose a grade with higher ESCR
PP
PP: heat resistance and clarity
Polypropylene withstands higher temperatures than HDPE and gives glossy, translucent bottles. Random copolymer and clarified grades give the best clarity.
Properties
- Suitable for hot filling at about 85 °C, depending on the grade
- Glossy surface; clarified grades are nearly transparent
- Lower density than HDPE: more bottles per kg
- Less impact resistant in the cold than HDPE
Typical containers
- Hot-fill sauces, syrups and juices
- Pharmaceutical and oral liquid bottles
- Translucent cosmetic bottles
- Wide-mouth jars with dome trimming
Processing notes
- Runs on the HDPE screw at higher barrel temperatures
- Narrower processing window and lower melt strength: keep parisons short and temperatures stable
- Crystallizes slower: allow longer cooling than for HDPE
- Higher post-mold shrinkage in the first 24 h; measure volume after one day
Common problems
- Hazy bottles: mold too warm or wrong grade; use a clarified grade and colder mold
- Parison sag: lower the melt temperature and shorten the parison
PVC
PVC: clear and stiff bottles
Rigid PVC gives clear, stiff bottles with good oil resistance. It is heat-sensitive and must not stay too long at high temperature.
Properties
- Clear and glossy
- Stiff, good resistance to oils and many chemicals
- High density: heavier bottles for the same wall
Typical containers
- Clear household and cleaner bottles
- Glue bottles
- Cosmetic and toiletry bottles
Processing notes
- Needs a PVC screw and die head with streamlined flow channels and a hard, corrosion-resistant surface
- Narrow temperature window; overheating releases HCl and degrades the material
- Purge with PE before stopping the machine; never leave PVC in a hot barrel
Common problems
- Yellow or black streaks: degraded material; lower temperatures and clean the die head
- Brittle bottles: check the stabilizer and processing temperature
PETG
PETG: glass-like clear bottles with handles
Extrusion blow molding grades of PETG give glass-like clarity in shapes stretch blow molding cannot make, such as integrated handles and offset necks.
Properties
- Very high clarity and gloss
- Good chemical resistance for cosmetics and personal care
- Tough, does not shatter
Typical containers
- Clear cosmetic and toner bottles
- Personal care bottles with handles
- Thick-base premium bottles
Processing notes
- Must be dried, typically about 65 °C for 4 – 6 hours in a dehumidifying dryer
- Use a PETG-type screw and die (KSY45-J1.8L)
- Thick bases need long cooling; typical cycles are 25 s or more
- Polished mold cavities for a clear surface
Common problems
- Hazy or bubbly bottles: material not dry enough
- Sticking to the mold: lower the mold temperature or blow time
LDPE
LDPE: soft squeeze bottles
Low-density polyethylene is soft and flexible. It is used where the bottle must be squeezed to dispense the product.
Properties
- Soft and squeezable
- Good chemical resistance
- Lower stiffness: not for stacking or heavy loads
Typical containers
- Eye-drop and dropper bottles
- Squeeze bottles for sauces and glue
- Laboratory wash bottles
Processing notes
- Lower processing temperatures than HDPE
- Often blended with HDPE to adjust stiffness
- Small bottles run on multi-cavity heads on the KSY50-J2L
Common problems
- Bottles too soft: add HDPE to the blend or increase wall thickness
Multilayer
Multilayer structures
Co-extrusion combines several materials in one wall. Each layer comes from its own extruder and the layers join in the die head.
| Structure | Layers, outside to inside | Used for |
|---|---|---|
| Three layers with regrind | HDPE / regrind / HDPE | Uses more regrind while keeping new material on the surfaces |
| Light-blocking three layers | White HDPE / black HDPE / white HDPE | UHT milk and light-sensitive products |
| Six-layer barrier | HDPE / regrind / tie / EVOH or PA / tie / HDPE | Agrochemicals, solvents, food that needs an oxygen barrier |
| View stripe | Transparent stripe in a colored wall | Engine oil bottles and cans, to show the fill level |
EVOH and PA do not bond to polyethylene, so a thin tie layer (adhesive resin) is placed on each side. The barrier layer is only a few percent of the wall, but it decides whether the container passes the permeation test. See our multilayer machines.
Resin grades
Choosing the right resin grade
Use a grade made for extrusion blow molding. Injection molding grades flow too easily and the parison sags.
- Small and medium HDPE bottles use blow molding grades with a low melt flow rate, typically below 1 g/10 min (190 °C / 2.16 kg).
- Jerry cans and drums need high-molecular-weight HDPE (HMW-HDPE) with very high melt strength, specified by the high-load melt index (190 °C / 21.6 kg). It carries the heavy parison and gives the drop and stacking strength.
- Detergent and chemical bottles need a grade with good environmental stress crack resistance (ESCR).
- Food and pharmaceutical containers need grades approved for food contact or medical use in your market.
- PP for clear bottles: random copolymer or clarified grades; for hot filling: grades with higher heat resistance.
Additives and regrind
| Material | Melt temperature | Mould temperature | Drying | Shrinkage | Regrind |
|---|---|---|---|---|---|
| HDPE | 175 – 205 °C | 10 – 16 °C | Not required | 1.5 – 2.5% | 20 – 30% single layer; up to 70% in a core |
| PP (homopolymer or clarified) | 195 – 220 °C | 15 – 25 °C (45 °C for hot fill) | Not required | 1.5 – 2.5%, more across a wide panel | Up to 30% on hidden parts |
| PVC (rigid) | 170 – 190 °C | 10 – 20 °C | Required for some compounds | 0.4 – 0.8% | Low, typically below 10% |
| PETG | 200 – 225 °C | 8 – 14 °C | Required: 65 – 70 °C, dew point −20 °C | 0.2 – 0.6% | Dry before use; below 20% on visible parts |
| LDPE | 160 – 185 °C | 10 – 18 °C | Not required | 1.5 – 3% | 20 – 30% |
Typical ranges for extrusion blow molding grades. A material outside its window fails in a predictable way: too cold gives unmelted particles and a rough surface, too hot gives sag and a weak weld line.
Masterbatch, additives and regrind
- Color masterbatch is typically added at 1 – 3 % by a dosing unit on the hopper. Opaque white and light-blocking colors need more.
- UV stabilizers protect containers stored outdoors, such as agrochemical cans and drums.
- Regrind from crushed flash is mixed back with new material. Many producers keep it below 20 – 30 % in single-layer containers; in a three-layer wall it can be the middle layer.
- Keep regrind clean and dry. Dust, mixed materials and moisture cause holes, streaks and weak spots.
Choose by product
Which material for which product
The product inside decides the material: chemical resistance, barrier, filling temperature and the look you want.
| Product in the container | Recommended material |
|---|---|
| Water-based chemicals, detergents, bleach | HDPE, single layer |
| Solvent-based agrochemicals and chemicals | HDPE with PA or EVOH barrier, multilayer |
| Fresh milk and juice | HDPE, single layer |
| UHT milk and light-sensitive drinks | HDPE, three-layer light-blocking |
| Hot-fill sauces and syrups | PP |
| Engine oil and lubricants | HDPE, often with a view stripe |
| Pharmaceutical tablets and oral liquids | HDPE or PP, medical grade |
| Clear cosmetics and personal care | PETG or PVC; PP for translucent |
| Squeeze and dropper bottles | LDPE or LDPE/HDPE blend |
| Jerry cans and drums, 5 – 25 L | HMW-HDPE |
FAQ
Material questions
Which material should I use for my bottle?
It depends on the product inside, the look you want and the filling temperature. Most bottles and cans are HDPE; hot-fill products need PP, clear bottles PETG or PVC, and solvents a multilayer barrier. Tell us the product and we suggest the material and layer structure.
Can one machine run several materials?
Yes. HDPE, LDPE and PP run on the same screw with different temperature settings. PVC needs a PVC screw and die, and PETG needs a dryer and is best on the KSY45-J1.8L.
How much regrind can I use?
Many producers keep regrind below 20 – 30 % of the blend in single-layer containers. In three-layer containers regrind can form its own middle layer between two layers of new material.
Why does PETG have to be dried?
PETG absorbs moisture from the air. Wet material breaks down in the extruder and gives hazy, bubbly or brittle bottles. A dehumidifying dryer at about 65 °C for 4 – 6 hours prevents this.
Why do bottles change size after molding?
Polyethylene and polypropylene keep shrinking for up to a day after molding, about 1.5 – 3 % for HDPE. The mold is made oversize to compensate, and the volume is checked on bottles that have rested 24 hours.
What is the difference between EVOH and PA barrier layers?
EVOH is an excellent oxygen barrier for food and pharmaceuticals but loses performance when wet. PA is used mainly as a barrier against solvents in agrochemical and chemical containers.
Do I need special HDPE for jerry cans?
Yes. Jerry cans and drums use high-molecular-weight HDPE with high melt strength, so the heavy parison does not sag and the can passes drop and stacking tests.
Can the same mold be used for HDPE and PP?
Often yes, but PP and HDPE shrink differently, so the volume and some dimensions change. For tight volume tolerances, the mold is made for one material.
Get a quote
Ask about your material
Tell us the material grade and the container. We confirm the screw, die head and settings.